A study of natural-pigment color masterbatches examined whether four commercial colorants—blue spirulina, yellow curcumin, red beetroot and green chlorophyllin—could survive melt processing in polylactic acid (PLA) and polybutylene succinate (PBS).
The researchers compounded the colorants into masterbatches by twin-screw extrusion, adding titanium dioxide, calcium carbonate and stearic acid to support UV protection, dispersion and processing. The masterbatches were diluted into the corresponding polymer at 2, 4 and 6 wt% and injection molded into test specimens.
Thermal window shapes the results
Natural pigments are organic and may degrade at lower temperatures than the polymers that carry them. Thermogravimetric analysis put onset temperatures at about 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot. PLA and PBS showed considerably higher degradation temperatures, so the team selected profiles that melted each matrix while limiting pigment exposure.
PBS was processed at up to 145 °C and PLA at up to 190 °C. The twin-screw extruder ran at 65 rpm and a feed rate of 2 kg/h. Most pigment-polymer pairs fit this window. Spirulina did not: it lost its blue color during PLA processing, so a blue PLA masterbatch could not be produced. In PBS, the lower temperature preserved enough pigment stability for compounding.
Flow and mechanical effects are modest
The pigments caused only limited changes in rheology. Melt flow rate fell slightly, pointing to a modest rise in melt viscosity. Neat PLA measured about 50 g/10 min, and its natural-pigment masterbatches stayed close to that value. PBS showed a similar, small reduction. The study says this matters for compounders because a color system that requires major screw, pressure or molding changes has little practical value; here, conventional twin-screw compounding and injection molding handled most formulations.
The researchers also checked tensile and impact behavior and found no significant overall losses across the 2–6 wt% range. PLA began at a Young's modulus of about 1,710 MPa and tensile strength of 65.6 MPa; PBS began at about 392 MPa and 34.5 MPa. The colored formulations remained near those baselines, while impact strength stayed in a similar range with some variation between pigments.
Light stability remains the main barrier
Extrusion success did not guarantee durable color. After 50 hours of xenon-lamp exposure, most formulations exceeded a color difference of Delta E* = 2, a level indicating visually perceptible change. The exception was a PLA formulation with 2 wt% green chlorophyllin masterbatch, which showed the highest photostability.
The study identifies UV stability as the largest obstacle to wider use. Packaging, consumer products, agricultural parts and outdoor applications may need extra stabilization, protective coatings or pigment modification before natural colors can compete with conventional systems over long service life.
The environmental comparison favored the natural route under the study's assumptions: 1 kg of curcumin pigment generated about 0.04 kg CO2-eq, versus 18.65 kg CO2-eq for an inorganic green reference pigment. The natural-pigment masterbatches also used less electricity during extrusion and pelletizing. Even so, the study concludes that lightfastness and thermal stability need further development; several colorants can be compounded into PLA and PBS on conventional equipment with limited flow and mechanical penalties.